性能項(xiàng)目 | 試驗(yàn)條件[狀態(tài)] | 測(cè)試方法 | 測(cè)試數(shù)據(jù) | 數(shù)據(jù)單位 | |
基本性能 | 吸水量 | 浸泡均衡點(diǎn)+73℉(+23℃) | ASTM D570 | 0.90 | % |
吸水量 | Equil.50%R.h.+73℉(+23℃) | ASTM D570 | 0.22 | % | |
密度 | ASTM D792 | 1.42 | |||
吸水量 | 24hrs浸泡+73℉(+23℃) | ASTM D570 | 0.25 | % | |
物理性能 | 絕緣強(qiáng)度 | Short Time,90 mils | ASTM D149 | 500 | V/mil |
絕緣系數(shù) | 系數(shù) +73℉(+23℃)102to106Hz | ASTM D150 | 3.7 | ||
絕緣強(qiáng)度 | Short Time,2.3mm | ASTM D149 | 19.7 | MV/m | |
擴(kuò)散因數(shù) | +73℉(+23℃)106Hz | ASTM D150 | 0.005 | ||
摩擦系數(shù) | +73℉(+23℃)靜態(tài) | 0.20 | ThrustWasherTest3 | ||
摩擦系數(shù) | +73℉(+23℃)動(dòng)態(tài) | ThrustWasherTest3 | 0.35 | ||
電阻系數(shù) | +73°F(+23℃)0.2%H2O | ASTM D257 | 1015 | ohm-cm | |
機(jī)械性能 | 伸張強(qiáng)度 | +122℃ | ASTM D638 | 26.2 | MPa |
撓曲系數(shù) | +212℉ | 在25℃下 | 130 | MPsi | |
彎曲降服強(qiáng) | +23℃ | ASTM D790 | 98.6 | MPa | |
撓曲系數(shù) | +122℃ | 在25℃下 | 620 | MPa | |
伸張強(qiáng)度 | +212℉ | ASTM D638 | 5.2 | Mpsi | |
lzod沖擊強(qiáng)度 | +23℃ | ASTM D256 | 123 | j/m | |
洛氏硬度 | ASTM D785 | M94,R120 | |||
斷裂時(shí)之拉力伸張度 | +158℉(+70℃) | ASTM D638 | 230 | % | |
伸張強(qiáng)度 | -55℃ | ASTM D638 | 101 | MPa | |
撓曲系數(shù) | -68℉ | 在25℃下 | 530 | MPsi | |
撓曲系數(shù) | -55℃ | 在25℃下 | 3650 | MPa | |
無(wú)切口沖擊程度 | +23℃ | D256 | >5300(no break) | j/m | |
撓曲系數(shù) | +70℃ | 在25℃下 | 1550 | MPa | |
撓曲系數(shù) | +250℉ | 在25℃下 | 90 | MPsi | |
壓縮應(yīng)力 | 縮應(yīng)力 +73°F@1%Def. | ASTM D695 | 5.2 | MPsi | |
彈性系數(shù) | +23℃ | ASTM D638 | 3100 | MPa | |
彎曲降服強(qiáng) | +73℉ | ASTM D790 | 14.3 | MPsi | |
lzod沖擊強(qiáng)度 | 40℃ | ASTM D256 | 96.1 | j/m | |
撓曲系數(shù) | +73℉ | 在25℃下 | 380 | MPsi | |
伸張強(qiáng)度 | +100℃ | ASTM D638 | 35.9 | MPa | |
壓縮應(yīng)力 | +23℃@10%Def. | ASTM D695 | 124 | MPa | |
彈性系數(shù) | +73℉ | ASTM D638 | 450 | MPsi | |
斷裂時(shí)之拉力伸張度 | -68℉(-55℃) | ASTM D638 | 38 | % | |
無(wú)切口沖擊程度 | +73℉ | ASTM D256 | >100(no break) | ft.lb/in | |
壓縮應(yīng)力 | +23℃@1%Def. | ASTM D695 | 35.9 | MPa | |
斷裂時(shí)之拉力伸張度 | +212℉(+100℃) | ASTM D638 | >260 | % | |
lzod沖擊強(qiáng)度 | -40℉ | ASTM D256 | 1.8 | ft.lb/in | |
伸張強(qiáng)度 | +23℃ | ASTM D-638 | 68.9 | MPa | |
負(fù)載下之變形 | 2000psi@+122℉(14Mpa@50℃ | ASTM D621 | 0.5 | % | |
伸張強(qiáng)度 | -68℉ | ASTM D638 | 14.7 | MPsi | |
撓曲系數(shù) | +23℃ | 在25℃下 | 2620 | MPa | |
伸張強(qiáng)度 | +158℉(+70℃) | ASTM D638 | 6.9 | MPsi | |
伸張強(qiáng)度 | +70℃ | ASTM D638 | 47.5 | MPa | |
彎曲疲勞忍耐限度 | +73℉ | ASTM D671 | 4.7 | MPsi | |
伸張強(qiáng)度 | +73℉ | ASTM D638 | 10.0 | MPsi | |
壓縮應(yīng)力 | +73°F@10%Def. | ASTM D695 | 18.0 | MPsi | |
剪力 | +73℉ | ASTM D732 | 9.5 | MPsi | |
撓曲系數(shù) | +100℃ | 在25℃下 | 895 | MPa | |
剪力 | +23℃ | ASTM D732 | 65.5 | MPa | |
拉力沖擊抵抗力 | +73℉ | D1822Long | 170 | ft.lb/in2; | |
斷裂時(shí)之拉力伸張度 | +73℉(+23℃) | ASTM D638 | 75 | % | |
伸張強(qiáng)度 | +250℉ | ASTM D638 | 3.8 | MPsi | |
lzod沖擊強(qiáng)度 | +73℉ | ASTM D256 | 2.3 | ft.lb/in | |
拉力沖擊抵抗 | +23℃ | D1822Long | 350 | KJ/m2 | |
彎曲疲勞忍耐限度 | +23℃ | ASTM D671 | 32.4 | MPa | |
撓曲系數(shù) | +158℉ | 在25℃下 | 225 | MPsi | |
斷裂時(shí)之拉力伸張度 | +250℉(+122℃ | ASTM D638 | >260 | % | |
電氣性能 | 電弧抵抗力 | 120mil(3.1mm) | ASTM D495 | 220no tracking | Sec. |
熱性能 | 熔點(diǎn) | ASTM D2133 | 347 | °F | |
熱變形溫度 | 1.8MPa | ASTM D648 | 136 | ℃ | |
線性熱膨脹系數(shù) | +85 to +140℉ | ASTM D696 | 6.8 | 10-5in/in.℉ | |
線性熱膨脹系數(shù) | +140 to +220℉ | ASTM D696 | 7.6 | 10-5in/in.℉ | |
線性熱膨脹系數(shù) | -40 to +85℉ | ASTM D696 | 5.8 | 10-5in/in.℉ | |
線性熱膨脹系數(shù) | -40 to +29℃ | ASTM D696 | 10.4 | 10-5m/m.℃ | |
熱變形溫度 | 264psi | ASTM D648 | 277 | ℉ | |
線性熱膨脹系數(shù) | +60 to +104℃ | ASTM D696 | 13.7 | 10-5m/m.℃ | |
熔點(diǎn) | ASTM D2133 | 175 | ℃ | ||
熱傳導(dǎo)系數(shù) | 0.37 | W/mk | |||
熱變形溫度 | 0.5Mpa | ASTM D648 | 172 | ℃ | |
熱傳導(dǎo)系數(shù) | 2.6 | BTU-in/hr | |||
線性熱膨脹系數(shù) | +220 to +300℉ | ASTM D696 | 8.3 | 10-5in/in.℉ | |
熱變形溫度 | 66psi | ASTM D648 | 342 | ℉ | |
線性熱膨脹系數(shù) | +104 to +150℃ | ASTM D696 | 14.9 | 10-5m/m.℃ | |
線性熱膨脹系數(shù) | +29 to +60℃ | ASTM D696 | 12.2 | 10-5m/m.℃ | |
其它性能 | 可燃燒性 | UL94 | 94HB |
基本簡(jiǎn)介
POM(聚甲醛樹脂)定義:聚甲醛是一種沒有側(cè)鏈、高密度、高結(jié)晶性的線型聚合物。按其分子鏈中化學(xué)結(jié)構(gòu)的不同,可分為均聚甲醛和共聚甲醛兩種。兩者的重要區(qū)別是:均聚甲醛密度、結(jié)晶度、熔點(diǎn)都高,但熱穩(wěn)定性差,加工溫度范圍窄(約10℃),對(duì)酸堿穩(wěn)定性略低;而共聚甲醛密度、結(jié)晶度、熔點(diǎn)、強(qiáng)度都較低,但熱穩(wěn)定性好,不易分解,加工溫度范圍寬(約50℃),對(duì)酸堿穩(wěn)定性較好。是具有優(yōu)異的綜合性能的工程塑料。有良好的物理、機(jī)械和化學(xué)性能,尤其是有優(yōu)異的耐摩擦性能。俗稱賽鋼或奪鋼,為第三大通用塑料。
(2)它具有耐疲勞、耐蠕變、耐磨、耐熱、耐沖擊等優(yōu)良的性能,且摩擦系數(shù)小,自潤(rùn)滑性好.
(3)POM不易吸濕,吸水率為0.22~0.25%,在潮濕的環(huán)境中尺寸穩(wěn)定性好,其收縮率為2.1%(較大),注塑時(shí)尺寸較難控制,熱變形溫度為172℃,聚甲醛有均聚甲醛兩種,性能不同(均聚甲醛耐溫性好一點(diǎn)).
加工工藝
1.POM加工前可不用干燥,好在加工過(guò)程中進(jìn)行預(yù)熱(80℃左右),對(duì)產(chǎn)品尺寸的穩(wěn)定性有好處.
2.POM的加工溫度很窄(0~215℃),在炮筒內(nèi)停留時(shí)間稍長(zhǎng)或溫度超過(guò)220℃時(shí)就會(huì)分解,產(chǎn)生刺激性強(qiáng)的甲醛氣體.
3.POM料注塑時(shí)保壓壓力要較大(與注射壓力相近),以減少壓力降.螺桿轉(zhuǎn)速不能過(guò)高,殘量要少;
4.POM產(chǎn)品收縮率較大,易產(chǎn)生縮水或變形.POM比熱大,模溫高(80~100℃),產(chǎn)品脫模時(shí)很燙,需防止?fàn)C傷手指.
5.POM宜在“中壓、中速、低料溫、較高模溫”的條件下成型加工,精密制品成型時(shí)需用控制模溫
6.POM具高機(jī)械強(qiáng)度和剛性
7.POM高的疲勞強(qiáng)度
8.POM環(huán)境抵抗性、耐有機(jī)溶劑性佳
9.POM耐反覆沖擊性強(qiáng),良好的電氣性質(zhì),復(fù)原性良好,具自已潤(rùn)滑性、耐磨性良好,尺寸安定性優(yōu).
聚甲醛樹脂 (POM) 是杜邦高性能聚合物事業(yè)部首款抗沖擊改性的 POM,可滿足汽車行業(yè)對(duì)內(nèi)飾塑料的嚴(yán)格要求。這將 Delrin? 聚甲醛樹脂在汽車中的應(yīng)用延伸到內(nèi)飾塑料部件,以應(yīng)對(duì)高沖擊負(fù)載的要求。
汽車工業(yè)
聚甲醛在汽車工業(yè)中的應(yīng)用量較大。用聚甲醛制作的零件具有減少潤(rùn)滑點(diǎn)、耐磨、便于維修、簡(jiǎn)化結(jié)構(gòu)、提高效率、降低成本、節(jié)約銅材等良好效果。代替銅制作汽車上的半軸、行星齒輪等不但節(jié)約了銅,而且提高了使用壽命。在發(fā)動(dòng)機(jī)燃油系統(tǒng),POM可以制造散熱器水管閥門、散熱器箱蓋、冷卻液的備用箱、水閥體、燃料油箱蓋、水本葉輪、氣化器殼體、油門踏板等零件。
電子電器
由于聚甲醛的電耗較小,介電強(qiáng)度和絕緣電阻較高,具有耐電弧性等性能,使之被廣泛的應(yīng)用于電子電器領(lǐng)域。如可用聚甲醛制造電扳手外殼、電動(dòng)羊毛剪外殼、煤鉆外殼和開關(guān)手柄等,還可制造電話、無(wú)線電、錄音機(jī)、錄像機(jī)、電視機(jī)、計(jì)算機(jī)和傳真機(jī)的零部件、計(jì)時(shí)器零件,錄音機(jī)磁帶座。
其它方面
建筑:可做自來(lái)水龍頭、窗框、洗漱盆、水箱、門簾滑輪、水表殼體和水管接頭等。
農(nóng)業(yè)機(jī)械:手動(dòng)噴霧器部件,播種機(jī)的連接和聯(lián)運(yùn)部件,擠乳機(jī)的活動(dòng)部件,排灌水泵殼,進(jìn)出水閥座、接頭和套管等。還可用于氣溶膠的包裝、輸送管、浸在油中的部件及標(biāo)準(zhǔn)電阻面 板等。
能克服純聚 四氟乙烯易
POM具有很低的摩擦系數(shù)和很好的幾何穩(wěn)定性,特別適合于制作齒輪和軸承。由于它還具有耐高溫特性,因此還用于管道器件(管道閥門、泵殼體)